Chemical composition
Fe2.4 %
Zn0.12 %
P0.03 %
Cubalance
CuFe2P combines good electrical and thermal conductivity with higher strength for connector applications.
Standards: ASTM B888
CuFe2P | C19400 | CW107C
| Property | Metric | Imperial |
|---|---|---|
| Electrical conductivity | 37 MS/m | 64 % IACS |
| Thermal conductivity | 260 W/(m.K) | 150 Btu.ft/(ft2.h.deg F) |
| Coefficient of electrical resistance | 3.3 10^-3/K | 1.8 10^-3/deg F |
| Coefficient of thermal expansion | 17.6 10^-6/K | 9.8 10^-6/deg F |
| Density | 8.91 g/cm3 | 0.322 lb/in3 |
| Modulus of elasticity | 121 GPa | 17,500 ksi |
| Specific heat | 0.385 J/(g.K) | 0.092 Btu/(lb.deg F) |
| Poisson's ratio | 0.34 | 0.34 |
Structured values for quote review, engineering checks and PDF generation.
| Standard | Temper | Rm MPa | Rm ksi | Rp0.2 MPa | Rp0.2 ksi | A50 % | Hardness | Grain size mm |
|---|
Graph series are generated from the same alloy technical config used for the PDFs.