Chemical composition
Cu60-63 %
Znremainder
Ni17-19 %
Sn0.03 max %
Fe0.3 max %
Pb0.03 max %
Mn0.5 max %
C76400 is a nickel silver offering medium-to-high strength, excellent hardness, good formability, corrosion resistance and solderability. It is a suitable alloy for connectors and relays; excellent corrosion resistance allows use in demanding environments.
Standards: ASTM B122/B122M
CuNi18Zn20 | C76400 | CW409J | NS107 (close) ≈ C77000 (CW409J)
| Property | Metric | Imperial |
|---|---|---|
| Melting point | 1060-1110 deg C | |
| Density | 8.72 g/cm3 | |
| Specific heat | 0.383 kJ/(kg.K) | |
| Thermal conductivity | 33 W/(m.K) | |
| Electrical conductivity | >=6 % IACS | |
| Modulus of elasticity | 125 GPa | |
| Coefficient of thermal expansion | 17.7 10^-6/K |
Structured values for quote review, engineering checks and PDF generation.
| Standard | Temper | Rm MPa | Rm ksi | Rp0.2 MPa | Rp0.2 ksi | A50 % | Hardness | Grain size mm |
|---|
Graph series are generated from the same alloy technical config used for the PDFs.